Power connections
Tin-Plated Busbar or Electroless Nickel
Use tin to ASTM B545-13 Class A or Class B when the part stays under the tin page's temperature line. Use electroless nickel at 0.1 to 3.0 mils when the joint needs that even coat.
On this page
Use tin when the part stays under the tin page's temperature line and the spec is ASTM B545-13, Class A (.0001) or Class B (.0002). As of November 7, 2026, Storm's tin page says tin-plated bus bars have a low operating window because of a low melting point around 450°F, and that nickel would be suggested if components operate above those temperatures. Use electroless nickel when the coat is the ENP range of 0.1 to 3.0 mils with a uniform tolerance of ±0.00005, including a multilayer lamination that needs that even coat. As of the same day, the ENP page lists medium-phosphorus content at 5 to 8 percent and nickel content at 92 to 95 percent. Hussey's plated length lines are a separate finish choice on the silver flash and tin page.
The tin page prints a class, a melting line, and the substrates
The tin page opened November 7, 2026 calls tin the most versatile finish for copper bus bars and describes corrosion resistance, solderability, and a mirror-like appearance for bright tin. The spec block prints ASTM B545-13 and MIL-T-10727, then Class A (.0001) or Class B (.0002). The page does not print the word inch on that class line. Substrates listed for the tin are copper C11000 and aluminum 6101 T-61. The engineering notes say tin can be combined with lead, nickel, and silver for special applications, and they name lead-acid batteries for tin-lead and switchgear contacts for tin-silver. They say tin plating is susceptible to whiskering, and that a nickel underplating is recommended for low-voltage electronic equipment where the components are closely spaced. They say bright tin can be scratched if hardware is installed after plating, and that matte tin or nickel is recommended if visual appearance matters.
The temperature note is the line that points away from tin. As of November 7, 2026, the page says the operating window is low because the melting point is around 450°F, and that nickel would be suggested above those temperatures. It says nickel, not a thickness. The thickness and the phosphorus figures are on the electroless nickel page. The tin class figures stay in the form the tin page prints: Class A (.0001) and Class B (.0002). The ENP range stays in mils, which is the unit that page prints. This comparison does not convert one into the other.
Electroless nickel is the even coat, at 0.1 to 3.0 mils
The ENP page opened November 7, 2026 describes electroless nickel as a nickel alloy applied by chemical reduction rather than by electrical current. It says the coat is uniform because the deposit does not depend on current distribution, and it names multilayer laminations and parts with irregular shapes, threads, and holes as the fit. It says Storm can produce ENP in a thickness range of 0.1 to 3.0 mils, set by the corrosion resistance the part needs, with a uniform tolerance of ±0.00005. The process it offers is medium-phosphorus ENP, also called bright high-speed ENP on that page. The property table lists nickel content 92 to 95 percent and phosphorus content 5 to 8 percent. The page says the process is lead-free and cadmium-free, and that the bath is pumped through a 5-micron filter.
Hardness is printed in two places that do not use one number. As of November 7, 2026, a sentence says heat treatment hardens medium-phosphorus electroless nickel as high as 68 Rockwell C, at 150 kg. The property table's after-plating row says 45 to 51 Rockwell and 500 to 600 Knoop. The after-heat-treating row says 64 to 71 Rockwell and 850 to 1000 Knoop. Copy the sentence when the request quotes the sentence, and copy the table row when the request quotes the table. As of November 7, 2026, other table cells are a plating rate of 12 to 30 microns per hour, a deposit density of ±8.1 grams per cubic centimeter, a Taber wear index of 16 to 20, and an electrical resistance of 40 to 70 µOHMcm. The page spells the reducing agent as sodium hypophosphate.
| Item | Tin page | Electroless nickel page |
|---|---|---|
| Spec or process | ASTM B545-13 and MIL-T-10727 | Medium phosphorus, 5 to 8 percent, nickel 92 to 95 percent |
| Thickness as printed | Class A (.0001) or Class B (.0002) | 0.1 to 3.0 mils, tolerance ±0.00005 |
| Temperature note | Melting point around 450°F | Heat treatment hardness sentence and the table rows |
| Where the page points | Nickel, if the part runs above that melting line | Multilayer laminations and irregular shapes |
| Substrate named | C11000 copper and 6101 T-61 aluminum | Copper bus bar, including a ground bar in the process steps |
The silver page adds a nickel strike under ASTM B700
Storm's silver page, opened November 7, 2026, is titled to ASTM B700. It says the ASTM B700 certification mandates a nickel strike before the silver. It describes a cyanide-free silver process with adhesion over copper and over nickel, with a strike plate. It says the cyanide-free plate has higher microhardness and a lower wear rate than cyanide-inclusive silver, and it does not print a hardness number for that comparison. It also says the cyanide-free plate tarnishes slightly more than cyanide silver, and that tarnish still occurs on both. A silver-flash length of 72 inch to 240 inch is Hussey's line, on the silver-flash page. Storm's silver page does not print that length.
The tin page's switchgear note, tin-silver, and the silver page's nickel-strike requirement are different sentences. As of November 7, 2026, tin-silver is an example of a combined finish on the tin page. The nickel strike is a requirement the silver page attributes to ASTM B700. A request for silver copies ASTM B700 and the nickel strike from the silver page. A request for tin copies Class A or Class B from the tin page. A request for electroless nickel copies 0.1 to 3.0 mils and the phosphorus cell from the ENP page.
What to copy onto the finish line
- Finish: tin, electroless nickel, or ASTM B700 silver, from the page opened November 7, 2026.
- Tin: ASTM B545-13, MIL-T-10727, Class A (.0001) or Class B (.0002), and bright or matte.
- Tin temperature: the melting line around 450°F, and nickel if the part operates above it.
- Electroless nickel: 0.1 to 3.0 mils, tolerance ±0.00005, phosphorus 5 to 8 percent, nickel 92 to 95 percent.
- Hardness: the 68 Rockwell C sentence, or the table's 45 to 51 and 64 to 71 Rockwell rows, kept as separate lines.
- Silver: ASTM B700 with the nickel strike the silver page says that standard mandates.
- Substrate for tin: C11000 or 6101 T-61.
Questions these plating pages answer
What does the tin page print for thickness?
Class A (.0001) or Class B (.0002), under ASTM B545-13 and MIL-T-10727, as of November 7, 2026. The page does not add the word inch on that line. The ENP thickness is printed in mils, 0.1 to 3.0, on the other page.
Which Rockwell number is the heat-treated coat?
The sentence says as high as 68 Rockwell C at 150 kg, as of November 7, 2026. The table's after-heat-treating row says 64 to 71 Rockwell and 850 to 1000 Knoop. Both lines are on the ENP page. Copy the line the request names.
When does the silver page require nickel?
The silver page says ASTM B700 mandates a nickel strike before the silver, as of November 7, 2026. That strike is the silver-page requirement. The tin page's nickel suggestion is the line for a part that operates above a melting point around 450°F.
Sources
Tin class, the melting line, whisker and underplate notes, and the C11000 and 6101 T-61 substrates are from Storm's tin page. Thickness, tolerance, phosphorus, nickel content, and the hardness lines are from Storm's electroless nickel page. The ASTM B700 nickel-strike sentence is from Storm's silver page. All three were opened November 7, 2026.